  "record_id": "dbbe764919636591",
  "title": "Success Case on Surface Finish for Hip Femoral Stems │ DLyte",
  "kind": "reference",
  "company": "DLyte",
  "parameters": {
    "Record type": "Application case study",
    "Process": "Dry electropolishing",
    "Workpiece": "Hip femoral stems",
    "Material": "Milled stainless steel",
    "Surface target": "Mirror finish",
    "Reported roughness": "Ra <0.03 µm",
    "Recorded batch size": "24 pieces",
    "Recorded process time": "64 min per batch",
    "Revised workflow": "Hand-belt preparation plus DLyte finishing",
    "Former workflow": "Belts, plastic media, nutshell media, hand polishing and waste handling",
    "Preservation requirement": "Tight tolerances, geometry, upper hole and laser marks"
  },
  "summary": "A dry-electropolishing route for milled stainless-steel hip femoral stems replaced belt, plastic-media, nutshell-media, hand-buffing and waste-handling stages with hand-belt preparation followed by automated finishing. The case reports 24 stems processed in 64 minutes and surface roughness below Ra 0.03 µm while preserving laser marks and geometry.",
  "sections": [
    {
      "heading": "Application and former route",
      "paragraphs": [
        "The workpieces are milled stainless-steel hip femoral stems. Their former finishing sequence used hand belts, plastic abrasive media, nutshell media, final hand buffing and a separate waste-handling stage.",
        "The project sought a mirror surface while avoiding changes to functional geometry and markings."
      ]
    },
    {
      "heading": "Qualified result",
      "paragraphs": [
        "The revised route consists of hand-belt preparation followed by dry electropolishing. The recorded case reports a 64-minute cycle for a batch of 24 stems.",
        "Measured surface roughness was reported below Ra 0.03 µm. Laser markings and the upper hole were retained, and the case identifies homogeneous finishing and tolerance preservation as critical acceptance points."
      ]
    },
    {
      "heading": "Production controls",
      "items": [
        "Document the milled starting roughness and belt-preparation condition for every validated lot.",
        "Use fixtures that expose required surfaces without damaging seating or reference features.",
        "Inspect laser marks, upper-hole coverage and transition radii after finishing.",
        "Verify roughness and dimensional tolerances rather than relying on gloss alone."
      ]
    },
    {
      "heading": "Safety and validation",
      "paragraphs": [
        "Maintain media condition, electrical contacts and fixture cleanliness according to the qualified process. Prevent cross-contamination between alloys and manage spent electrolyte under the applicable waste procedure.",
        "Medical implants require controlled validation beyond surface appearance. The archived case does not define sterilization, implant release criteria or a universal cycle for other stem designs."
      ]
    }
  ],
  "updated_at": "2026-10-13T08:34:42.874Z"
}