Success Case on Carbide Insert Polishing │ DLyte
This cutting-tool case addresses dry electropolishing of tungsten-carbide inserts while controlling cobalt-binder leaching and edge geometry. A former robotized diamond-brushing route taking about 10 minutes per insert was replaced by a batch process reported at 40 inserts in 10 minutes; the project roughness target was Ra below 0.01 µm.
Technical profile
| Manufacturer / publisher | DLyte |
|---|---|
| Record type | Application case study |
| Process | Dry electropolishing |
| Workpiece | Tungsten-carbide cutting inserts |
| Material system | Tungsten carbide with cobalt binder |
| Project roughness target | Ra <0.01 µm |
| Former process | Robotized diamond brushing and diamond-disc grinding |
| Former polishing time | About 10 min per piece |
| Recorded batch size | 40 pieces |
| Recorded batch time | 10 min |
| Primary risks | Cobalt-binder leaching, uncontrolled edge rounding and geometry loss |
| Downstream context | Surface preparation before final coating |
| Category | Chemical & special polishing |
| Updated | 2026-10-13T08:34:42.874Z |
Material challenge
Tungsten carbide is difficult to polish mechanically without rounding cutting edges. Chemical or conventional electrochemical routes can also remove cobalt binder from the carbide structure, creating a leaching risk.
The case therefore treats surface improvement, edge control and binder retention as separate acceptance requirements.
Former and revised processes
The former route used a robotized arm with diamond-loaded brushes followed by a diamond-disc grinding operation, with about 10 minutes of polishing time per insert.
The dry-electropolishing batch route was reported to process 40 inserts in 10 minutes. The project target was Ra below 0.01 µm; because another summary value on the captured page is less stringent, the target is retained as a project objective rather than presented as a universal guaranteed result.
Quality controls
- Measure roughness and edge radius independently; a glossy face does not demonstrate edge preservation.
- Inspect for binder depletion, pits and color changes that could indicate an unsuitable cycle.
- Confirm laser marks and part identity after processing.
- If a coating follows, qualify adhesion and cutting performance on the complete coating stack.
Process safety and maintenance
Segregate media used for carbide grades from other alloys and monitor electrolyte condition over its qualified life. Clean fixtures and confirm reliable electrical contact before each batch.
Use the current machine and consumable safety instructions. The case data does not replace tool-life trials for a specific carbide grade, edge preparation or coating system.